Lithium Tantalate (LiTaO3)
 |
 |
|
| Basic Properties |
| Crystal Structure |
Trigonal, Space group R3c, Point group 3 m |
| Cell Parameters |
A = 5.154 Å |
C = 13.781 Å |
| Melting Point |
1650 °C |
|
| Curie Temperature |
607 °C |
|
| Mohs Hardness |
5.5 |
|
| Density |
7.46 g/cm³ |
|
| Dielectric Constant |
?e11 / ?e0 51.7 |
?e33 / ?e0 44.5 |
| Elastic Stiffness Coefficient |
CE11 2.33 ( X 1011 N/m² ) |
CE33 2.77 ( X 1011 N/m² ) |
| Piezoelectric Strain Constant |
d22 2.4 ( X 10-11 C/N ) |
d33 0.8 ( X 10-11 C/N ) |
| Transmission Range |
400 – 4500 nm |
|
| Electro.optical coefficients |
r33 = 30.4 pm/V |
|
| Refractive index at 632.8 nm |
n0 = 2.176 |
ne = 2.180 |
| |
| Typical SAW Properties |
| Cut Type |
vs (m/s) |
k2s (%) |
TCV (10-6 / °C) |
TCD (10-6 / °C) |
| X-112° Y |
3295 |
0.75 |
-16.50 |
22.3 |
| Y-Z |
3230 |
0.66 |
|
35 |